Home/Materials

Materials

Proprietary materials, specified in numbers.

Lightweight aluminium and magnesium, high- to full-density steels, and SMTiC carbide. Property values below are typical and come from Sinter Metal's own data.

Lightweight solutions

New-generation aluminium.

Lighter parts can improve energy efficiency in use, reduce the power needed for the same performance, and help customers work toward new efficiency regulations.

Full-density, precipitation-hardened aluminium equivalent to 7075, with an optional SiC reinforcement for extreme wear resistance.

PropertyHardened steel (C50)Aluminium (6061)7075 PM aluminiumSiC PM aluminium
Density (g/cm³)7.802.702.812.80-2.84
Tensile strength (MPa)590180-230570570
Hardness (HB)181-26965165-185165-185
Wear resistanceHighLowMediumExtreme
Corrosion resistanceMediumHighHighHigh
Heat resistanceMediumLowLowHigh
MachinabilityYesYesYesYes
Pricing--Competitive*Competitive*

* Comparable to steel part pricing. Aluminium-steel parts are in serial production for home appliances: high productivity, stable SPC and Cpk, homogeneous material, net or near-net shape.

Ultra-light

Magnesium alloy parts.

Full-density magnesium parts: ultra-light yet strong.

Density1.80 g/cm³
Tensile strength350 MPa
HardnessAs specified

High- to full-density steel

Replace bar-stock machining.

HD parts replace steel parts machined from bar stock, with guaranteed homogeneity and (near) net shape, at much lower cost and with a stable process.

When designing HD parts, define the fracture and fatigue requirement (tensile strength, hardness) and the toughness requirement (yield strength, hardening process).

GradeHD3 ConventionalHD2 OptimalHD1 SuperiorFull density
Density (g/cm³)7.20-7.407.30-7.507.50-7.707.80
HardeningSinter-hardening or case-hardeningSinter-hardening or case-hardeningSinter-hardening or case-hardeningSinter-hardening or case-hardening
ApplicationIncreased strength and fatigue resistance. Not for high-torque or superior-strength requirements.High hardness, high toughnessMost demanding requirements
Part designRequires balanced stress/strain distributionDoes not require balanced stress/strain distribution
Dimensional controlImproves from HD3 to full density

SMTiC

A tougher carbide at less than half the weight.

SMTiC is a titanium-carbide composite. TiC particles are about 30% harder than tungsten-carbide particles, and a steel binder (50% of volume, against 6-15% cobalt in WC) gives far higher toughness without losing hardness. At full density of 6.4 g/cm³ it weighs less than half as much as most WC composites.

PropertyWC compositesSMTiC
Density (g/cm³)14-156.4
Hardness (HRA)87-9085-86
Wear resistanceGoodExtreme
Corrosion resistance at high temperatureAverageVery good
ToughnessBrittleVery high
Pricing-Competitive (comparable to other carbides)

HRA: Rockwell A hardness (ISO 6508). WC values are typical for cemented carbide grades.

Steel-mill rolling

SMTiC parts run in steel rolling at about 1,100 °C with abrasion, corrosion and stress, and significantly outperform WC parts there.

Press tooling

Our own PM press tools face repeated compression and crack-inducing stress. SMTiC is our material of choice for wear- and crack-resistant, low-maintenance tools.